| Test Item | Test unit | Physical Standard | |||||
| Thickness | mm | 1.50' | |||||
| Width | inch | 54 | |||||
| Rupture Strength | Long. | N(1cm) | ¡Ý200 | ||||
| Lat. | N(1cm) | ¡Ý200 | |||||
| Elongation% | Long. | 2.5cm | ¡Ý60 | ||||
| Lat. | 2.5cm | ¡Ý60 | |||||
| Tear Strength | Long. | N(3cm) | ¡Ý90 | ||||
| Lat. | N(3cm) | ¡Ý90 | |||||
| Racking Strength | Long. | N(3cm) | ¡Ý105 | ||||
| Lat. | N(3cm) | ¡Ý105 | |||||
| Normal temp. sinuation tolerance | Long. | 200,000 times | No fissure | ||||
| Lat. | 200,000 times | No fissure | |||||
| Low temp. sinuation tolerance | Long. | -20¡æ 80,000 times | No fissure | ||||
| Lat. | -20¡æ 80,000 times | No fissure | |||||
| Yellow color change £¨UV 4 Hours£© | 250mm 30W | ¡Ý3.5 | |||||
| Breaking Strength | Kg/cm2 | ¡Ý30 | |||||
| After hydrolyze Racking Strength | Long. | (3cm) N | ¡Ý100 | ||||
| Lat. | (3cm) N | ¡Ý100 | |||||
| ¡¡ | ¡¡ | ¡¡ | Physical Standard of Micro Fiber Lining | ¡¡ | ¡¡ | ¡¡ | ||
| Thickness (mm) | Weight (g/m2) | Rupture Strength £¨N/3cm£© | Elongation% | Tear Strength £¨N/3cm£© | Racking Strength £¨N/3cm£© | anti-hydrolyze £¨N/3cm£© | Breaking Strength £¨N/3cm£© | Remark |
| 0.60¡À0.05 | 200¡À20 | ¡Ý30 | ¡Ý40 | ¡Ý20 | / | / | ¡Ý7.0 | grinding |
| 0.80¡À0.05 | 320¡À20 | ¡Ý80 | ¡Ý50 | ¡Ý50 | / | / | ¡Ý12 | |
| 1.20¡À0.10 | 440¡À50 | ¡Ý120 | ¡Ý50 | ¡Ý60 | ¡Ý80 | ¡Ý80 | ¡Ý16 | |
| 1.20¡À0.10 | 500¡À50 | ¡Ý150 | ¡Ý50 | ¡Ý85 | ¡Ý80 | ¡Ý80 | ¡Ý18 | ¡¡ |
| 1.40¡À0.10 | 520¡À50 | ¡Ý180 | ¡Ý60 | ¡Ý100 | ¡Ý100 | ¡Ý100 | ¡Ý25 | ¡¡ |
| 1.60¡À0.10 | 650¡À50 | ¡Ý200 | ¡Ý60 | ¡Ý100 | ¡Ý100 | ¡Ý100 | ¡Ý25 | ¡¡ |
| 1.80¡À0.10 | 700¡À50 | ¡Ý200 | ¡Ý60 | ¡Ý100 | ¡Ý90 | ¡Ý80 | ¡Ý25 | ¡¡ |
| 2.00¡À0.10 | 820¡À50 | ¡Ý200 | ¡Ý60 | ¡Ý160 | ¡Ý90 | ¡Ý80 | ¡Ý35 | ¡¡ |